技(ji)術交流
電話:
手(shǒu)機:
郵箱:@cn01.cc
地(di)址:山東龍(long)口市東中🔞文在线中文资源❌江(jiang)街道政府(fu)南雅居苑(yuan)臨街樓307号(hào)
當前(qián)位置: 首頁(yè) > 技術交流(liu) > 電鍍常用(yòng)知識
電鍍銀(yin)沉積速度(dù)
(電流(liú)效率為100%時(shí))
電鍍(du)時間(min) | 0.2A/dm2 | 0.3 A/dm2 | 0.5 A/dm2 | 0.7 A/dm2 | 1.0A/dm2 | |
1um | 7.9 | 5.3 | 3.2 | 1.1 | ||
15.8 | 10.5 | 6.3 | 4.5 | 2.1 | ||
3um | 23.7 | 9.5 | 6.8 | 3.2 | ||
5um | 39.5 | 26.4 | 15.8 | 7.9 | 5.3 | |
55.3 | 36.9 | 22.2 | 15.8 | 11.0 | 7.4 | |
9um | 71.1 | 47.6 | 28.4 | 14.2 | ||
10um | 79.0 | 31.6 | 15.8 | 11.0 | ||
30um | 237 | 158 | 68.0 | 47.0 | ||
50um | 395 | 158 | 113.0 | 79.0 | 53.0 | |
80um | 632 | 422 | 181 | 84.0 | ||
100um | 790 | 527 | 230 | 158 | 110 |
電鍍(dù)錫沉積速(sù)度
(電(dian)流效率為(wéi)%時)
時(shí)間(min) | A/dm2 | 0.5 A/dm2 | 0.6 A/dm2 | A/dm2 | A/dm2 | 1.0 A/dm2 | 1.2 A/dm2 | 1.5 A/dm2 | |
1um | 18.9 | 14.2 | 9.4 | 8.1 | 7.1 | 4.7 | 3.8 | ||
22.7 | 14.2 | 11.3 | 9.4 | 7.5 | |||||
3um | 56.6 | 42.5 | 28.3 | 24.3 | 21.3 | 17.0 | 14.1 | 11.3 | |
4um | 57.0 | 45.3 | 38.0 | 32.0 | 28.0 | 22.6 | 15.0 | ||
5um | 94.0 | 71.0 | 47.0 | 40.0 | 35.4 | 28.3 | 23.6 | 18.8 | |
113 | 68.0 | 57.0 | 34.0 | 28.3 | 22.6 | ||||
7um | 132 | 99.0 | 79.0 | 66.0 | 57.0 | 39.6 | 33.0 | 26.4 | |
113 | 76.0 | 65.0 | 45.0 | 38.0 | 30.0 | ||||
9um | 170 | 127 | 102 | 85.0 | 73.0 | 51.0 | 43.0 | 34.0 |
電鍍鉻(ge)沉積速度(dù)
(電流(liú)效率為13%時(shi))
電鍍(du) 時間(jian)(min) | 10 A/dm2 | 15 | 25 A/dm2 | 40 A/dm2 | 50 A/dm2 | A/dm2 | A/dm2 | |||
1um | 9.81 | 6.53 | 3.92 | 3.26 | 2.80 | 2.45 | 1.96 | 1.63 | 1.22 | 0.98 |
2um | 19.6 | 13.1 | 6.54 | 5.60 | 4.90 | 3.92 | 3.92 | 2.45 | 1.96 | |
19.6 | 11.8 | 8.41 | 7.35 | 5.88 | 4.90 | 3.68 | ||||
4um | 39.2 | 26.1 | 15.7 | 13.1 | 9.80 | 7.85 | 6.55 | 3.92 | ||
49.1 | 19.6 | 16.3 | 14.0 | 12.3 | 9.81 | 4.91 | ||||
58.9 | 23.5 | 19.6 | 14.7 | 11.8 | 5.89 | |||||
7um | 68.7 | 27.5 | 22.9 | 19.6 | 17.2 | 13.7 | 11.5 | 8.58 | 6.87 | |
8um | 78.5 | 52.3 | 26.2 | 22.4 | 19.6 | 13.1 | 9.81 | |||
9um | 58.8 | 35.3 | 29.4 | 22.1 | 17.7 | 14.7 | 11.0 | 8.83 | ||
10um | 98.1 | 39.2 | 32.7 | 28.0 | 24.5 | 19.6 | 16.4 | 12.3 |
電鍍鎳沉(chen)積速度
(電流效(xiao)率為%時)
電鍍 | 0.8 A/dm2 | 1.0 A/dm2 | 1.2 A/dm2 | 1.5 A/dm2 | 2.0 A/dm2 | 2.5 A/dm2 | 3.0 | 4.0 | |
1um | 10.3 | 6.4 | 5.1 | 4.3 | 2.1 | 1.7 | 1.3 | ||
2um | 20.5 | 10.2 | 8.6 | 5.1 | 4.1 | 3.4 | 2.6 | ||
31 | 19.2 | 15.4 | 12.8 | 7.7 | 6.2 | ||||
4um | 41 | 25.6 | 20.5 | 17.1 | 10.3 | 8.2 | 6.8 | 5.1 | |
5um | 51 | 32 | 21.4 | 17.1 | 8.6 | 6.4 | |||
10um | 51 | 43 | 34 | 25.6 | 17.1 | 12.8 | |||
15um | 154 | 96 | 77 | 64 | 51 | 38 | 25.7 | ||
20um | 103 | 86 | 68 | 41 | 34 | 25.6 | |||
256 | 160 | 128 | 85 | 64 | 51 | 43 | 31 | ||
30um | 308 | 192 | 128 | 103 | 77 | 51 | 38 | ||
40um | 171 | 103 | 68 | 51 | |||||
321 | 257 | 214 | 171 | 128 | 103 | 86 |
不(bu)同電流效(xiào)率的電鍍(du)金沉積速(sù)度
單(dān)位:um/h
60% | 70% | 80% | 90% | 100% | |
3.0 | 3.4 | 3.8 | |||
0.2A/dm2 | 4.5 | 5.3 | 6.8 | 7.6 | |
6.8 | 8.0 | 11.4 | |||
0.4A/dm2 | 9.0 | 10.6 | 12.2 | ||
13.3 | 17.1 | 19.0 | |||
0.6A/dm2 | 16.0 | 18.2 | 20.6 | 22.8 | |
0.8A/dm2 | 18.0 | 21.2 | 24.4 | 27.4 | 30.6 |
1.0A/dm2 | 22.6 | 26.6 |